Nichel-ferro Core Covered Welding Rod ENiFe-CI
AWS A5.15 ENiFe-Ci
IS01071-EC NiFe-Ci
JIS Z3253 DFCNiFe
GB/T 10044 EZNiFe-1
Type of Covering: Graphitemould
Welding Position: F,H,HF,OH,V
Type of Current: AC or DCEP
Features & Applications
ENiFe-Ci is a graphitic type coating with Nickel/Ferro core welding rod and it is machinable one. The rod is suitable for repairing or surfacing cracked and worm parts made of gray iron or nodular iron, as well as joining cast iron with dissimilar metals. Lower current is recommended to obtain better welding operation. Before welding the rod should be baked 1 hour at a temperature around 150°C.
Chemical Composition of Deposited Metal(%) – ENiFe-Ci
| C | Mn | Si | S | Ni | Al | Cu | Fe | Others | |
| Standard | ≤2.00 | ≤2.50 | ≤4.00 | ≤0.03 | 45-60 | ≤1.00 | ≤2.50 | Remain | ≤1.00 |
| Typical | 0.71 | 0.24 | 1.00 | 0.007 | 55.16 | 0.054 | 0.055 | 42.70 | 0.23 |
Size,Piece & Recommended Current(AC or DC⁺)
| Size(mm) | 2.5×300 | 3.2×350 | 4.0×350 | 5.0×350 | |
| Piece(1kg) | ≈55 | ≈33 | ≈22 | ≈14 | |
| Current(A) | 60-90 | 90-110 | 120-150 | 150-180 | |
Notice:
1. The rod should be baked at 80℃-120℃ for 1 hours before use.
2. The surfaces to be welded must be cleaned away impurities of oil contamination, rust, moisture and so on.
3. When welding, hammering the weld joint to dispel stress around the welding region to avoid crack.
4. To increase ability of crack-resisting and machinable, small current is recommended, meanwhile could reduce impurities to permeate the weld seam from base metal.